Downloaded from https://www.everyspec.com ) dry for an appreciable time, a nroiev'tive oxide film is 18. , , , formed which greatly reduces the rate of corrosion. 15A 12 months Controlled laboratory tests have shown that the air- 0m'h developed film protects iron from corrosion in clean air J14.0 at relative humidities as high as 99 percent. If, however, Z the film is exposed to 0.01 percent or more of sulfur 9 12.0 A A AMCP 706-117 dioxide at this high relative humidity, corrosion occurs. I Also, once the oxide film has been exposed to sulfur oo.9 6 months dioxide, it no longer pretects the surface against corro- I a sion in clean air at relative humidities of 80 percent and ' above.
60 A few seconds exposure to air is all that is needed for 3 months a 'stainless' chromium steel to develop an invisible ox. 4,0- ide film on its surface which renders it inert to most atmospheric pollutants. Parts made of stainless steel 2.0 located on the Empire State Building have been ex- posed for 30 yr with no loss of utility or beauty due to cp o.02 o.04 0.1.h Mi.l 60 0.112 0.j4 .16 0.18 corrosion (Ref. 28). MEAN SULFUR DIOXIDE CONCENTRATION. ppm Low carbon (0.019 percent) low copper (0.028 per- FIGURE 2-33.
Relationship Betwun Corrosion of cent) mild steel, because of its sensitivity to atmos- Mild Stool and Corrmponding Mon Sulfur Dioxide pheric corrosion, has been used in atmospheric corro- MildS n forrying Len Supour Piods ,ion studies (Ref. 44). Results from the tests show good Concentraon for Vaying Lenld Expoure Periods correlation between corrosion losses and sulfur dioxide concentrations, and little if any correlation between is re corrosion losses and dustfall or suspended particulate b at ielatey slow for humidities lower than 70 percent matter, Fig. 2-33 shows corrosion loss as a function of but accelerates markedly for values above approxi- sulur ioxde oncntrtios.
reresionanaysi of mately 80 percent. Laboratory studies using bare and sulfur dioxide concentrations. A regression analysis of varnished steel panels that were treated with a combi- these data yields the telationship. nation of various powdered oxides, salts, and dusts and then exposed to atmospheres of pure clean air and air Y = 54. 1 S + 9. 5 (2-21) containing sulfur dioxide (very low concentration but not specified) at various humidities produced the fol- lowing results (Ref. 13): where (1) Filiform corrosion, characterized by a filamen- Y corrosion weight loss, grams tal configuration, the primary phase in electrolytic cor- per hundred grams of panel (4 rosion, was noted in all cases.
X 6 X 0.035 in.) (2) For relative humidities less than about 70 per. S mean sulfur dioxide cent, corrosion rates are low but increase at higher concentration, ppm humidities.
The regression coemcient was statistically significant at the I-percent level, Suspended particulate matter (3) The addition of traces of sulfur dioxide to the measurements were made and analyzed for their con- test atmospheres greatly increased the rate of corrosion tribution to the corrosion loss, Statistical analyses in all instances, showed that the influence of sulfur dioxide was signifi- (4) In most cases corrosion increased with an in- cant wherei.s that of suspended particulate matter was crease in relative humidity even in clean air. not.
Dustfall measurements did not show a statistically significant correlation with corrosion rates, Analysis of exposure data for carbon steel shows that Results from other laboratory and field studies indi- increasing the level of oxidants actually retards the rate cate that particulate matter can be an important factor of corrosion (Ref. 45). Fig. 2.34 shows the relationship in the corrosion of metals, especially in the presence of between corrosion rate, sulfur dioxide concentration, sulfur dioxide, and oxidant concentration.
The ability of oxidants to The critical relative humidity for corrosion of ferrous decrease the corrosion rate can be caased (I) by inhibit- metals is between 70 and 80 percent. The corrosion rate ing the mechanism or (2) by improving the protective. 2.57