US Army Materiel Command AMCP 706-117 — Environmental Series, Part Three: Induced Environmental Factors (EN)

Downloaded from https://www.everyspec.com AMCP "/06-117? help explain the mechanlom of atmospheric corrosion of (5) Magnesium. The critical relative humidity for aluminum by sulfur dioxide. In Fig. 2-37 both types of magnesium is about 90 percent. For relative humidities aluminum show the same rate of corrosion at 52 percent above this value, magnesium hydroxide, believed to be relative humidity. This curve is very nearly the same as the primary corrosion product, is formed. The mag.

that for the oxidation of aluminum without sulfur di- nesium hydroxide absorbs carbon dioxide from the at- oxide, indicating that even high concentrations of sulfur mosphere to form magnesium carbonte (M#CO 3 ) and dioxide do not appreciably attack aluminum at low this in turn reacts slowly with sulfur dioxide to form relative humidities. Fig. 2-38 shows that at the higher magnesium sulfate (MgSO 4 ) (Ref. 47).

relative humidities at which these data were obtained, the rate of corrosion is greater initially but approaches zero after about 60 hr except for 3003 alloy at 85 2-7.4.3 Buildin Materials percent (note the chqnge from um to mg on the ordinate Building materials are affected by atmospheric pollu. scales when comparing Fig. 2.38 to Fig. 2-37). At 85 tants In a variety of ways. Perhaps the most familiar percent relative humidity the rate of corrosion for the effect is the soiling of buildings by particulate matter. 3003 alloy continues to increase even after 100 hr. At Tarry or carbonaceous materials resulting from ineffl.

the higher humidities (72 and 85 percent), analysis of clent combustion of soot-producing fuel are likely to be the white powdery deposit formed on the surface acidic as well m sticky. If these are not removed by rain showed it to be A1 2 (SO 4 )3 .18 H,0, which indicates or special wmshinp, they adhere to surfaces and can that sulfur dioxide plays an essential role In the corro. result In a physical-chemical degradation of the material sion of aluminum at high humidities. In addition to their soiling effects. (4) Nickel.

The characteristic fogging of a nickel Limestone (CaCO,) in the presence of moisture reacts surface produced by exposure to polluted atmospheres is with sulfur dioxide and sulfur trioxide to form calcium due to the simultaneous presence of sulfur dioxide and sulfate (CaSe 4 ) and gypsum (CaSO, .2lH2 0), both of water vapor (Ref. 47), The critical relative humidity Is which ar partially soluble in water. Also, carbon about 70 percent below which the nickel surface will dioxide in the presence of moisture produces carbonic remain bright Indefinitely.

At hunmidities greater than 70 acid that then converts limestone into a water-soluble percent, the catalytic oxidation of atmospheric sulfur bicarbonate that is then leached away. dioxide to sulfur trioxide by the nickel surface forms a dilute solution of sulfuric acid on the surface. In the 2-7.4.4 Textiles beginning stages of attack, the surface film can be re. moved by wiping. As corrosion progresses, the basic sul- A variety of natural and synthetic textile fibers are fate is precipitated and the film becomes adherent giving susceptible to damage by sulfur dioxide. Particulate the surface an etched appearance.

After exposing a matter acts as a soiling agent with deterioration occur- specimen to an Industrial atmosphere for 88 days, the ring mainly due to increased frequency of cleaning. surface film was shown to have the formula NiSO 4 '0.33 Outside exposure studies of cotton fabrics have shown NI(OH), upon analysis, a direct correlation between air pollution and the accel- Nickel panels exposed to rain do not corrode as rap- erated degradation of the fabric (Ref. 42). The primary idly as those that are sheltered. This is attributed to the means of sample evaluation used In these studies was to fact that rain washes the acidic solutions from the sur- measure the breaking strength retention.

Also, the face, keeping it comparatively uncontaminated and free degree of seoling on undyed samples was determined by from attack. It has also been shown that preexposure reflectance measurements. Results of the study showed a of the sample to an atmosphere containing hydrogen strong relationship between retained breaking strength sulfide will suppress corrosion. This effect is believed to and mean sulfation rate as shown In Fig. 2-39.

A similar be due to a poisoning of the catalytic activity of the relationship was observed between retained breaking surface and not to the formation of a protective surface strength and mean sulfur dioxide concentration as oxide film as has been the cae for other metals such as shown in Fig. 2-40. DustfaUl and suspended particulate Copper. measurements also vurmlated with fabric degradation Nickel parts of telephone crossbar switches corrode and soiling but not as weU as suifation rate and sulfur and form a bright.greenish corrfoion product. This Wn- dioxide concentration.

In heavily contaminated sites, the grates to the region of the switch contacts causing open degradation rate was four to five times that of the least circuits. The corrosion is promoted by the presence of polluted sites as shown by Flp. 2-39 and 240. anions, principally nitrates, in accumulated dust. 242