US Army Materiel Command AMCP 706-117 — Environmental Series, Part Three: Induced Environmental Factors

Downloaded from https://www.everyspec.com AMCP 706-117 400 0 300 II 20 200 40 40 100- :00 100 0 100 200 300 400 o00 -3 SULFUR DIOXIDE, V6 FIGURE 2-34. Effects of Sulfur Dioxide and Oxidant Concentrations of Depth of Corrosion of Carbon Steel Expoed for 10 -,r ness of the rust film. The corrosion rate is proportional and sulfur dioxide concentration as determined from to the sulfate accumulation in the oxide film. Such the study is given by accumulation occurs when the iron oxides react with sulfur dioxide to form sulfates.

If oxidants remove the sulfur dioxide from the reaction by oxidizing it to sulfur trioxide, then the rate of corrosion should decrease, Y = 0.001028(RH - 48.8)SOs, AM yr-1 thus explaining the data. Also, the protectiveness of the (2-22) oxide film is increased by oxidizing ferrous oxide and where magnetite to the more protective ferric oxide. y = zinc corrosion rate, tm yrf' RH = average relative humidity, % 2-7,4.2 Nonferrous Metals average SO 2 concenttion, AA m 3 The nonferrous metals, as with the ferrous metals, These results are graphically presented in Fig. 2-35. are ,ffected primarily by the presence of sulfur dioxide. Eq.

2-22 accounts for 92 percent ofthe variability in the The reactions involved in the effects are dependent on average zinc corrosion rates. The critical relative hu- The eacion inolve intheeffcts re epeden on midity for zinc in sulfur dioxide free air is approxi- the specific metals as is the degree of damage. The more maty 7prcen h owev e as E.2 indictesin commpn f tesemetas ae dscused n te flloing mately 70 percent; however, as E~q. 2-22 indicates, in common of these metals are discussed in the following the presence of sulfur dioxide, the surface will be wet sulparagraphs: and corrosion will occur at relative humidities down to (1) Zinc.

Zinc is used in galvanizing to protect fer- approximately 49 percent. The results of the study were rous metals from atmospheric corrosion but is itself used to predict the useful lif,. of galvanized products in subject to corrosion under certain conditions. The two different types of environments (see Table 2-22). variables most important in determining the amount of Nickel-brans wire springs used in telephone relays corrosion are relative humidity and atmospheric sulfur have been damaged by high nitrate concentrations in dioxide concentration. airborne dust (Ref. 8).

Nickel-brass wires, under mod- erate stress and with a positive electrical potential, suf- Special high-grade commercial zinc (99.9 percent fer a form of streu-corrosion cracking when surface pure) panels were exposed at eight rural and eight ur- nitrate concentrations are above 2.4 /g cm- 2 and when ban sites for periods of 4, 8,16, 32, and 64 mo (Ref. 46). the relative humidity is above 50 percent. The relative Weight-loss data, measured as grams per panel, were humidity is an important controlling factor. When zinc converted to corrosion rates in micrometers per year.

is left out of the nickel-brass alloy, stress corrosion no Sulfur dioxide concentrations and relative humidity longer occurs. were monitored for the duration of the test. The rela- (2) Copperandsilwr. Copper and copper alloys--in tionship among rate of corrosion, relative humidity, the absence of hydrogen sulfide and sulfur dioxide- 2-58