MIL-HDBK-304C e. Compress the specimens per paragraph 9.1.9.6 and record the compressive load(s), before aging (F b ), at the displacements(s) computed in step d. f. Age specimens for 14 days in environmental chamber. Unless otherwise specified, the chamber conditions should be 120 ± 2є F (49 ± 1є C) and 95 ± 5 % relative humidity. g. Dry the specimens for 24 hours at 120 ± 2є F (49 ± 1є C) in a mechanically-convected drying oven or environmental chamber. h. Condition specimens for at least 16 hours per paragraph 9.1.1.4. i. Compress specimens without further preworking per paragraph 9.1.9.6.
Use the thickness and displacements from steps d and e and record the compressive load(s) after aging (F a ) . 9.1.13.6 Calculation. Change in resistance to compression before and after aging should be calculated as follows: Compression resistance change (%) = F b - F a (100) (9:6) Fb where: Fb = compressive load after preworking but before aging Fa = compressive load at the same deformation after aging 9.1.14 Flexibility. 9.1.14.1 Scope. This procedure is used to check the cushioning material flexibility. 9.1.14.2 Apparatus. A cylinder or mandrel with a diameter three times (+10 percent) the thickness of the specimen will be required for this test. 9.1.14.3 Test Specimen.
Each test specimen should be a strip of the cushioning material with a length approximately 12 times its thickness and a width one half its length. 9.1.14.4 Conditioning. Test specimens must be conditioned per paragraph 9.1.1.4. Specimens to be tested at other than ambient conditions must be conditioned at the test temperature for a period of 4 hours immediately preceding the test. The test cylinder should be conditioned for at least 1/2 hour immediately preceding the test at the same conditions specified for the test specimens. 9.1.14.5 Test Procedure. The specimen should be bent snugly around the mandrel through a total angle of 180 degrees.
The specimen should be examined for failure while it is in place on the mandrel. Failures such as cracking, delamination, surface spalling, or any other failure should be noted. 9.1.15 Contact Corrosivity Test. 9.15.1 Scope. The package designer must insure that the cushioning material will not react with the container or the item so as to cause corrosion. The contact corrosivity test is commonly used to determine if the cushioning material may cause corrosion. 9.15.2 Test Procedure. See FED-STD-101, Test Method 3005, “Contact Corrosivity Testing for Packaging Materials”, as an example of a test procedure. Other test procedures may be acceptable. Check with the procuring activity.
82 Downloaded from https://www.everyspec.com