MIL-HDBK-304C 9.1.10 Tensile Strength. 9.1.10.1 Scope. This procedure is used to check compliance of the cushioning material tensile strength with a minimum strength requirement. 9.1.10.2 Test Procedure. Refer to ASTM D 1623, “Standard Test Method for Tensile and Tensile Adhesion Properties of Rigid Cellular Plastics”. Follow specification test procedure and report format. Use of the compression/tension testing machine shown in Figure 9-7 is required. 9.1.11 Fragmentation. 9.1.11.1 Scope. This procedure is used to measure the dusting and fragmentation characteristics of commonly used cushioning materials. 9.1.11.2 Test Procedure.
Refer to ASTM C 421, “Standard Test Method for Tumbling Friability of Preformed Block Type Thermal Insulation”. Follow specification test procedure and report format. 9.1.12 Fungus Resistance. 9.1.12.1 Scope. This procedure is designed to show if a material is subject to attack by fungi. Cushioning material is sprayed with a standard test fungi suspension of mixed spores. Specimens are observed for fungus growth while stored under conditions of elevated temperature and humidity. 9.1.12.2 Test Procedure. Refer to ASTM G 21, “Standard Practice for Determining Resistance of Synthetic Polymeric Materials To Fungi”. Follow specification test procedure and report format.
9.1.13 Hydrolytic Stability. 9.1.13.1 Scope. This procedure determines the change in static compressive strength of cushioning specimens at room temperature that are subjected to high temperature and humidity conditions over an extended period of time. 9.1.13.2 Apparatus. The apparatus required for this test is as follows: a. An environmental chamber of a suitable size to hold the specimens and capable of maintaining the required temperature and humidity over an extended period of time. b. A balance or scales with an accuracy of ± 0.01 pound (± 5 grams). c. A compression/tension testing machine similar to the one in Figure 9-7. 9.1.13.3 Test Specimens.
The specimens should be per paragrah 9.1.9.3. 9.1.13.4 Conditioning. Test specimens should be conditioned per paragraph 9.1.1.4. 9.1.13.5 Test Procedure. a. Measure and record specimen length, width, and thickness per paragraph 9.1.2. b. Weigh and record specimen weight to within 0.01 pounds (5 grams). c. Prework specimens per paragraph 9.1.16. d. Compute the displacement(s) for the required strain(s) before aging. 81 Downloaded from https://www.everyspec.com