Bombardier Recreational Products Inc. (BRP) Sea-Doo RXT iS255 GTX LIMITED — Print Preview - C:\DOCUME~1\coderma\LOCALS~1\Temp\.aptcache\smr2009Piranhaen6/tfa03092

Section 07 BODY AND HULL Subsection 02 (BODY) then additional reinforcement may be necessary. This subject will be covered in COMPOUND FRACTURES. buffing with a white medium compound. Finish off using a fine compound. While buffing, pay close attention to avoid overheating the surface. Preparing the Surface Small Fractures: Open the cracks up with a sharp triangular can opener or preferably a car- bide tipped die grinder. The V groove will provide a good bonding area for the gelcoat. With 220-grit sandpaper, sand the sides of the notched out ar- eas. Numerous Fractures: Using a grinder with a 24-grit disk, remove the gelcoat. Sand the area edge with 220-grit sandpaper.

Compound Fractures Repair Possible causes: Thickness of fiberglass laminate Direct result of impact. Compound fractures are those that have gone past the gelcoated surface and in through the lay- ers of fiberglass laminate. Two types of repairs have to be performed. The first is to restore the structural integrity of the damaged area. Fracture types can vary from a simple crack to a large hole. Usually, fiberglass reinforcement becomes necessary, especially if the fracture can be at- tributed to weakness. The final part of the repair is the gelcoating, which cannot be done until the interior and exterior laminate surfaces have been repaired. Outside:

Remove the damaged gelcoat and fiber- glass with a 24-grit disk using a power sander. Grind outward at least 2 inches from the fracture to allow the patch to bond to strong material. Cut enough pieces of fiberglass mat necessary to build up the area. The pieces should be cut so they overlap each other by at least a half inch. For a smoother finish, the last layer should be fiberglass cloth. If the fracture is small enough all you may have to do is fill the area with an epoxy filler. Inside: For the interior repair, you can grind more. This will allow for more fiberglass material which will strengthen the area.

If the fracture opening is too large after surface preparation, you may need a backing support to cover the opening. Cut alter- nating pieces of fiberglass mat and cloth in over- lapping sizes. Filling the Repair Area Small Fractures: Refer to the same procedure as in the AIR BUBBLES. Numerous Fractures Over Large Surface: Pre- pare the area for spray application of liquid gel- coat. Wipe down the surface with acetone. Mask the area off to protect the watercraft from over- spray. Mix the needed quantity of gelcoat and catalyst according to suppliers recommendations. The gelcoat can be thinned with acetone up to 10%. If it needs more consistency you can add cabosil.

Make sure that the air supply is free of oil, dirt and water. Test spray the gelcoat mixture on paper to verify its consistency and pattern. You may have to ap- ply 5 or 6 coats to cover the area properly. Over- lap each coat further than the last, leaving at least 30 seconds between passes. Avoid trying to coat the surface with only a few heavy coats, this will not allow the gelcoat to dry properly. Apply a coat of polyvinyl alcohol (PVA) to seal off the air and protect the gelcoat surface from dust. PVA speeds up the curing process because gel- coat will not cure properly when exposed to air. Patching the Repair Area Outside: The outside should be done first.

Wipe clean the area with acetone on a cloth, then mask off area. For a small crack use an epoxy filler in the same way you would use gelcoat repair putty. When laying up a larger area you will use mat, cloth and fiberglass resin and catalyst. Use a clean container to mix the resin, mix only what you will need. Follow the recommended catalyst ratio. Using a clean paintbrush, brush the mixed resin on the surface. Place the smallest piece of mat over the fracture and then wet out the mat. Fol- low with the remaining pieces of mat and final layer of cloth. While wetting the pieces make sure you work the air bubbles out and saturate all the Sanding Wash the polyvinyl alcohol off with water.

De- pending on the size of the area repaired, you can either block sand as per previous procedure or you may use an air sander. Sand the surface down with progressively finer grits of sandpaper until the desired finish is achieved. Buffing and Waxing Buff the surface using a heavy duty polisher with a buffing pad. Make sure the pad is free of dirt or you may damage the gelcoat. Carefully begin smr2009-042 495